top of page

PHOTO #4 Removed tube sample

NOTE: Failure in tube
PHOTO #4
Bottom Half - Note Minimal Corrosion
Liquid
PHOTO #5 Severe groove depth adjacent
to edge of support

PHOTO #6

PHOTO #7

PHOTO #8

PHOTO #5
Top Half - Note Corrosion

PHOTO #6
Bottom Half - Note Minimal Corrosion

PHOTO #7 Cross Section
Tube split to show top & bottom
-
Left & right sides show minimal corrosion. Liquid covered.
-
Inner left & right (top circumference of tube) show heavy corrosion. Liquid/Vapor.

PHOTO #8
Top Half - Note Corrosion

Unexpected Tube Failure in
HDS Stripper OVHD Air Cooler
chronicle companion images

PHOTO #2

NOTE: Close up of Failure
PHOTO #1
Top half of tube looking at failure
PHOTO #3
Top Half of Tubing - Note Corrosion
Liquid/Vapor